Lesson 2 of 8

Rot, stain, mould and insects: telling damage apart

Not all fungal damage is equal

Distinguishing the types of damage tells you how urgent a problem is and what it costs.

Damage What it does Effect
Brown rot Degrades mainly cellulose and hemicelluloses; brittle, brown, cube-cracked residue Rapid early strength loss; mostly attacks softwoods; the most economically important decay in temperate building timber
White rot Degrades lignin and cellulose; bleached, stringy wood Typical of hardwoods; strength loss comparatively slow at first
Soft rot Attacks wood in permanently moist conditions such as soil or cooling towers Relevant where wood stays wet
Blue stain (sapstain) Fungi live on sugars in the sapwood and colonise fresh logs and green timber quickly Mainly disfigurement; costs grade
Mould Surface growth of spores on damp wood Often confined to the surface; costs grade; some moulds can cause respiratory problems in sensitive people

"Brown rot in softwoods, white rot in hardwoods" is a tendency, not a law. Stain and mould cost grade; only rot destroys structure.

A common yard test (general practice): rub the surface. Mould smears or brushes off; blue stain is in the wood and does not.

Stain timing: why the mill must be fast

Figures from the US Wood Handbook storage chapter (North American conditions):

  • Blue stain can develop in the sapwood of exposed log ends within 2 weeks after felling in warm weather.
  • Discoloration can penetrate into the log at up to about 30 cm (1 ft) per month. This is a maximum, not a typical rate.
  • Wood at 25-30 % MC, solid-piled in warm weather, can show stain within a week.
  • Stain fungi grow best at about 21-32 degrees C in wood above 22 % MC, are dormant below about 10 degrees C and, per a trade source, die above about 54 degrees C.

Insects in general terms

Insects have a different timeline from fungi. The Wood Handbook chapter says insects are inactive at or below about 10 degrees C and that activity roughly doubles with each 5-6 degrees C rise, reaching a maximum near 27 degrees C. Ambrosia beetles are usually a minor hazard in lumber stored away from forests or sawmills. Powder-post beetles are particularly damaging to large-pored hardwoods such as oak and ash. European durability sheets classify timber against two beetles as simply susceptible (S) or durable (D).

Worked example: a warm-season storage plan

You saw pine boards in July. Antistain dip treatments have limited safe times before the board must dry: 1 day at 27 degrees C or above, 2 days at about 21 degrees C, 1 week at about 15 degrees C and 1 month at about 10 degrees C.

  • Daily temperature is 27 degrees C: after a dip the boards must be drying within 1 day.
  • Stickered boards under a roof will not reach 20 % MC in a day, so the dip alone is not a plan. You also need prompt stickering and shelter.

Checklist for the yard

  • Move logs first-in, first-out; keep storage short in the warm season.
  • Use end coating, wet or sprinkled storage, or other listed options when logs must wait.
  • Sticker green boards promptly with dry stickers; do not close-pile wood above 20 % MC.
  • Keep sawn timber off the ground and protect it from rain.
  • After drying, wrap or shelter: kiln-dried wood stored outdoors in wet weather regains moisture, and stain-free packaging can stain later from condensation.
  • Never treat sapwood as durable.

Key points

  • Brown rot is the most damaging in temperate construction timber; blue stain and mould mainly cost grade, but only rot destroys structure.
  • Mould can usually be brushed off; blue stain is inside the wood.
  • In warm weather expect stain within days to about two weeks on exposed sapwood; at 25-30 % MC solid-piled it can appear in a week.
  • Antistain dips buy only limited time, from 1 day (warm) to 1 month (cool).
  • Insect activity rises with temperature and is negligible at or below about 10 degrees C.
  • Fast drying, good stacking and shelter are the mill's main protection.
Previous Next lesson

Sign in to save your progress and take the quiz. Sign in